Potassium Chloride Acid Zinc Plating

Delivery term:The date of payment from buyers deliver within days
  • Price:

    Negotiable

  • minimum:

  • Total supply:

  • Delivery term:

    The date of payment from buyers deliver within days

  • seat:

    Hubei

  • Validity to:

    Long-term effective

  • Last update:

    2017-12-18 04:01

  • Browse the number:

    352

Send an inquiries
Company Profile
Wuhan Fengfan Electroplating International Trading Co.,Ltd
Contactaixin:

fengfan(Mr.)  

Email:

telephone:

phone:

Arrea:

Hubei

Address:

3F No.8 LingjiaoHu Rd., Hankou, Wuhan 430015, China

Website:

http://www.fengfan-plating.com/ http://www.enhesh.com/com/fengfan/

Product details

Potassium Chloride Acid Zinc PlatingCLZN-10

 

I. Properties

1. It is composed of ClZn-10A and ClZn-10B, the deposit is white bright, the gloss-finishing is fast.

 

2. The bath has perfect ability of resisting iron impurities, suitable for both rack and barrel plating.

 

3. The deposit is fine and bright, easy for making passivation, such as color, blue-white and white.

 

4. Stable plating solution, low brightener consumption. 

                         


Rack plating

Barrel   plating

KCl

180~220g/L

200~240g/L

ZnCl2

60~70g/L

45~60g/L

H3BO3

30~35g/L

30~35g/L

ClZn-10A Brightener

1~2ml/L

0.4~1.5ml/L

ClZn-10B Bath make-up   agent

20~30ml/L

20~30ml/L

PH

4.5~5.5

5.0~6.0

Cathode current density(Dk)

0.5~3A/dm2

0.1~3A/dm2

Temperature

10~40

10~40

Anode

0zinc ingot

                          